The weld every wheel twists
Assumes The detail decides and the steel does not, The load that never came near failing anything and The internal force with no diagram.
The detail decides and the steel does not set out what a fatigue check contains: a stress range, a count of cycles, and a detail category, which is a statement about the geometry of a weld rather than about any material. Everything in it depends on the stress range being the right one. A detail category is calibrated against the nominal stress at the detail, in the direction that opens its crack, and a check made with a different stress — in the wrong direction, or from a model that cannot see the stress at all — is a check of a different detail.
Crane runway girders are where that goes wrong most often and most expensively. The weld that joins the web to the top flange directly under the rail is the classic site of their fatigue cracks, and the stress that cracks it is not the one a girder design produces. A girder is designed as a beam, and its web-to-flange weld is checked for the longitudinal shear and the girder’s bending, both of which a crossing crane cycles once. What cracks the weld is a stress across it: the web bending as a plate under each wheel, because the wheel does not stand on the web.
The torque that stops at the web
The torque a quarter of a rail makes followed the wheel’s eccentricity into the girder as a whole: a 180 kN wheel 18.75 mm off the web twists the girder by 3.4 kN·m, and the girder answers by bending its flanges sideways. That essay passed over a step. The torque does not arrive at the girder’s shear centre; it arrives on the top flange, through the rail, and the flange has to hand it to the web before the girder can do anything with it.
The flange is a plate 229 mm wide and 19.6 mm thick, and as a bar it is weak in twisting — its torsional constant is mm⁴. It sits on the web’s edge along its length, and the web holds it against turning. So locally, near the wheel, the top flange is a twisted bar resting on a continuous rotational spring, and the spring is the web bending as a plate out of its own plane. Where the flange is stiff, it spreads the wheel’s torque along the panel between web stiffeners, which hold it against twist; where the web is stiff, the web takes the torque close to the wheel and bends hard there to do it. The bending stress in the web plate at its top edge is greatest exactly at the toe of the fillet weld, in the direction across it.
EN 1993-6 gives the solution of that problem in closed form. With the torque , stiffeners a distance apart, a web of thickness and depth , and the torsional constant of what twists on top of the web,
The first factor in is the stress the torque would put into the web if it were spread evenly along the whole panel as plate bending. The second, , is how far it is from even. itself compares the web’s stiffness against twist to the flange’s: a small is a flange that spreads the torque, a large one a web that takes it close to the wheel.
The same competition between a flange and a web has been met before under the same wheel. The load that chooses its own length found that a crane wheel’s vertical load is spread along a girder’s web over an effective length that is an output of the flange’s bending stiffness against the web’s, not an input anybody chooses. The torque is spread the same way, by the flange’s torsional stiffness against the web’s resistance to being turned, and plays the part the effective length played there. The difference is in what the web does with whatever reaches it. A vertical load spread over a length squeezes the web in its own plane; a torque spread over a length bends it out of its plane, and a thin plate is far weaker in the second way than in the first: an 11.9 mm web that carries a wheel’s vertical load in compression without difficulty is bent to more than the girder’s own stress by a torque of 3.4 kN·m.
Bigger than the span
For the 612 × 229 mm girder with its 11.9 mm web and the rail loose on the flange, so that the flange twists alone, is 2.01 at a stiffener spacing of 2 m and the local stress at the weld is 139 N/mm². The girder’s bending stress under the same wheel at mid-span of its 8 m span is 113. A wheel that misses the web by three per cent of the girder’s depth bends the web at the weld harder than the whole span bends the girder.
The hero figure also shows how little the stiffener spacing matters. From 1 m to 6 m the local stress with a loose rail stays between 132 and 139 N/mm². Closer stiffeners concentrate the plate’s resistance into a shorter length, which raises the even-spread stress, and at the same time reduce , which lowers the concentration factor; the two nearly cancel. Stiffeners are put into crane girders for other reasons, and this is not one of them.
The figure’s other curve is the one that matters. If the rail is clipped to the flange tightly enough that the two twist together, the rail’s own torsional constant — about mm⁴ for an A75 rail, three and a half times the flange’s — joins the flange’s. falls to 0.95 and the local stress to 50 N/mm². The rail is the stiffest thing above the web, and whether it counts depends entirely on its fixings.
The number by hand
The 139 can be had in four lines, which matters because the formula looks opaque and the result is surprising enough to be doubted. The torque is N·mm. Spread evenly along a 2,000 mm panel as plate bending of an 11.9 mm web, it would give N/mm². The ratio is , the hyperbolic factor is 0.93, and , so and . The local stress is N/mm².
Written out like that, the result is visibly a product of two factors of the same size, neither of them small. The even-spread stress is already 71.5, two thirds of the girder’s bending stress, before any concentration — because a web 11.9 mm thick is a weak plate, and a torque of 3.4 kN·m along two metres of it is not a small moment for it to carry. The concentration then nearly doubles it.
The stiffness above the web decides
That makes the torsional constant above the web the variable to follow.
The flange alone, mm⁴, gives 139 N/mm². Flange and fixed rail, , give 50. A flange ten times as stiff in torsion gives 26. The curve is steep where it matters, between the flange alone and the flange with its rail, because that is where passes through one and the plate stops taking the torque locally.
This is the crane girder’s version of the stiffest path takes the load. The wheel’s torque has two ways to reach the stiffeners, and it divides between them by stiffness: along the flange as twist, or into the web as plate bending near the wheel. Every design choice that stiffens the first path — a thicker flange, a rail that is fixed rather than floating, a cap channel that closes a cell over the flange — moves the torque off the weld.
A millimetre off the web, again
The local stress is in proportion to the eccentricity, as the girder’s warping stress was, but at a much higher rate.
With the rail loose each millimetre the wheel runs off the web adds 7.4 N/mm² at the weld, nearly four times the 2.0 it added to the girder’s flange tips. The local stress equals the girder’s bending stress at 15.2 mm — inside the conventional quarter of the rail’s width, 18.75. With the rail fixed the rate is 2.7 N/mm² a millimetre and the crossing is at 42.1 mm, outside anything a sound runway should see.
So the same allowance means two quite different things depending on the rail’s fixings. With a fixed rail, the conventional eccentricity leaves the local stress well below the girder’s bending, and a worn rail or a poorly tracking crane has some room. With a loose one, the convention already puts the local stress above the bending, and wear goes straight onto the weld at seven newtons per square millimetre per millimetre.
The web that bends harder for being thicker
The obvious remedy for a web that bends too hard is a thicker web. It does not work the way it is expected to.
A thicker plate is stronger in bending, as the square of its thickness. It is also stiffer against the flange’s twist, as the cube, so it takes more of the torque near the wheel instead of leaving the flange to carry it away. The two act in opposite directions, and their ratio, through , decides. With the rail loose the stress at the weld is 141 N/mm² for an 8 mm web, peaks at 144 near 9.5 mm and is still 99 at 25 mm — more than doubling the web’s thickness from the girder’s 11.9 mm takes off less than a third. With the rail fixed the curve rises the whole way from 40 N/mm² at 8 mm to 53 at 15.5, and a thicker web there makes the weld’s stress worse.
That is the second refutation, and it is the kind of result that is unwelcome because it breaks a rule of thumb that is right almost everywhere else. A plate bent by a load bends less when it is thicker. A plate bent by a rotation imposed on its edge — which is what the twisting flange imposes on the web — bends more when it is stiffer, because a stiffer plate resists the rotation more and therefore takes more of the moment that produces it. Thickening the web is a strength remedy for what is, near the wheel, a compatibility problem.
The flange buys what the clip buys
The flange is a better place to spend steel.
The flange’s torsional constant grows as the cube of its thickness, so the web’s stress falls fast as the flange thickens: with the rail loose, 134 N/mm² at 20 mm, 60 at 30 and 30 at 40. A loose rail on a flange 32.3 mm thick gives the web what a fixed rail gives it on the girder’s 19.6 mm flange. Put the other way, the rail’s fixings are worth about thirteen millimetres of flange plate along the whole runway — which is a useful number when an existing girder’s rail clips are being chosen, and a reason why heavy crane girders are built up with thick top flanges or capped with channels rather than given thicker webs.
Counting the cycles at the weld
A fatigue check needs the cycles as well as the stresses, and here the two stresses differ again. The girder’s bending at the weld is one cycle per pass of a crane carriage: its influence line is a triangle over the span, and two wheels on one carriage, a few metres apart, add into one peak. The local web bending is one cycle per wheel: it exists only while a wheel is in the panel above the point, and returns to nothing between wheels. A two-wheel end carriage therefore gives the weld two local cycles and one global one each time it passes.
With a slope of three, damage goes as the cube of the range, so two local cycles of 139 N/mm² against one global cycle of 113 is a ratio of . The weld is dying of the stress the girder model does not contain, nearly four times as fast as of the one it does. With the rail fixed the ratio is 0.18, and the girder’s bending governs. The two are equal when the torsional stiffness above the web is twice the flange’s own, which is less than the rail would add if it were fixed. That is why the figure’s title is about the rail’s clips: they decide which of two stresses the weld’s life is spent on.
One honest caution about the figure. The two stresses meet the same weld in different directions — the local bending across the weld, opening a crack along it from the toe into the web; the girder’s bending along it — so they are counted as separate damage, not added into one range. Where both open the same crack, as at a weld toe where the flange and web stresses combine, a combined check is needed; the standard gives one, and this figure does not attempt it. And the absolute life depends on the detail category assigned to the weld in each direction, which depends on whether it is a fillet or a full-penetration weld and on how it is finished. The figure compares the two damages rather than predicting either.
What this check rests on
The closed form assumes a flange simply supported against twist at each stiffener and a web clamped at its far edge. Real stiffeners are not perfectly rigid and the bottom flange is not a clamp; both soften the web’s resistance slightly and so lower .
The eccentricity is the conventional quarter of the rail. It is the same allowance a weld group’s elastic share would be checked against, and it is not a measurement. The essay’s whole sensitivity to it is linear, and the true distribution of where wheels run on a rail is wider than a quarter of its width for a worn rail or a badly aligned crane.
The rail is either loose or fully fixed. Real clips grip with friction and some flexibility, and a rail on a resilient pad twists partly with the flange. The two curves are bounds.
The girder’s bending stress is its mid-span value under one wheel. Two wheels add at mid-span and raise the global range; the comparison of damage would then move toward the global stress, though not by the factor of the rail’s fixings.
A detail category is a direction
The general lesson is the one strongest across and first to crack across drew for weld groups, and the rule that points sideways for the direction a fatigue check reads: a weld’s fatigue strength belongs to a stress in a particular direction relative to the weld, and the stress a structural model produces may simply be in the wrong direction. The web-to-flange weld of a crane girder is checked, by its girder model, for stresses along it; it cracks under a stress across it that the model cannot produce, because the model’s girder has no width to its flange and no eccentricity to its wheel. The cure is not a better beam analysis. It is a second, local model, about a plate and a bar rather than a beam, run alongside the first.
And the comparison with the cycles that do not count goes the other way here. There, small cycles below a threshold did no damage. Here, the extra cycles are large, more numerous than the global ones and invisible to the global model — the opposite of cycles that do not count.
Still open: the rail clip that loosens
Every case here has the rail either loose or fixed for the girder’s whole life. Rail clips relax, pads compress and bolts lose their preload under the same wheels whose torque the clips were meant to share, and a rail that starts fixed can end loose. The local stress then rises, over the life, from the 50 N/mm² of a fixed rail toward the 139 of a loose one, and with it the damage per pass by a factor of twenty. Whether a fatigue check should be made at the end-of-life stiffness, or whether a runway’s inspection interval for its clips is in fact the variable that sets its welds’ life, needs a model of how clip preload decays under cycling — the question the joint that hides its clamp in its loop asked about bolts, which has not yet been asked about a rail.
Named alongside this one
Essays reaching for the same objects. Nobody chose these; they are what the concept index makes visible.
- The spectrum that only scales the girder detail category · fatigue · miners rule · stress range
- Which reversal closes the loop detail category · fatigue · miners rule · stress range
- Designed to be found in time detail category · fatigue · stress range
- How far a doubler has to run detail category · fatigue · fillet weld
- More hangers, and the same steel detail category · fatigue · stress range
- The bracing nobody took out detail category · fatigue · torsion
What links here
Every essay whose body links to this one.
The objects this essay names
Each one links to every other essay that touches it.
Crane girderDetail categoryEccentricityFatigueFillet weldMiners ruleStress rangeTorsionTorsional constant