The bend that finds the seam's line
Assumes The strength the welder gives back, The shear strength nobody measured and The worst stress is not where the worst bending is.
The seam that pressure protects took a seam winding round an aluminium tube and asked what its soft heat-affected zone could carry when the tube is pulled and pressurised at once. The zone is a thin band softened by the welding, held on both sides by stronger parent metal. Wherever the parent is far from its own yield, it fixes the band’s strain along the band’s own line, so the band has to yield across that line alone, and is lent strength by the restraint — the weld that is weakest at fifty-five degrees found the same band under a uniaxial pull. The one place the restraint lends nothing is where the seam lies along a line that the remote stress does not stretch. Under axial tension that line is at 54.7° to the axis. Under a closed tube’s own pressure, which pulls the wall round twice as hard as along, the only such line is the axis itself, so a seam at the 50 to 70 degrees that spiral mills use is helped: in 6082-T6 a 60° seam keeps 78 per cent of the tube’s strength.
A pipeline is rarely only pressurised, and the hoop stress that is only a radius times a pressure is not the only stress in its wall. It is laid over uneven ground, bent round curves, pulled by settlement, and the bend adds an axial stress that changes sign round the tube — tension on the outside of the bend, compression on the inside — while the pressure’s hoop stress stays the same all the way round. The essay ended by asking what that does to a seam that winds through every one of those loadings in each turn: whether the points where the seam crosses a line the local stress does not stretch are where it fails, whether those points move as the bend tightens, and whether a point that is only briefly on the line can still borrow its neighbours’ help.
A tube held at pressure, and then bent
The tube is 6082-T6, the parent’s ultimate strength 310 N/mm² and the welded zone’s 185, the alloy of the earlier essays. The seam is at 60° to the axis. The pressure is held at a level that makes a hoop stress of 100 N/mm², with the closed ends adding half that along the axis; then the tube is bent, and the bending stress at its outermost fibres is raised until something reaches its strength. The parent is checked by von Mises, the criterion behind a shear strength nobody measured; the seam’s soft zone by the band condition, at every point of a turn, with the stresses at that point. Whichever is reached first, at whatever point, ends the tube.
The figure sets the two cases side by side. Under pressure alone the seam keeps 78 per cent of the parent’s strength at every pressure, because a pressure’s stresses are all in proportion and the ratio does not depend on how large they are. In bending, with the pressure held, the seam keeps 60 per cent if there is no pressure, 56 per cent at a hoop stress of 100 N/mm² and 50 per cent at 175. The protection pressure gave has not merely been lost under the bend; pressure now makes the seam worse.
The 60 per cent with no pressure is the seam’s uniaxial share. A bent tube with no pressure has, at its most stretched fibre, a plain axial tension, and a 60° seam is close to the 54.7° at which uniaxial tension lends a band nothing. The earlier essay found that a 60° seam keeps 60 per cent of the tube’s strength in axial tension, and the bend’s outermost fibre is an axial tension.
The line the bend brings back
Why the pressure, which protected the seam, makes the bend worse is a question about the unstretched line, and it can be followed as the bend grows.
A wall in plane stress has a line it does not stretch only when one principal strain is a lengthening and the other a shortening — when its circle of strain, drawn as the circle nobody draws draws stress, crosses zero. Under a closed tube’s pressure the wall lengthens round its circumference and, very slightly, along its axis, so the only line left unstretched is the axis itself. Bending adds axial stress on the stretched side and the wall’s axial strain grows. While the axial stress is between half the hoop stress and twice it, the wall lengthens in every direction and has no unstretched line at all; that is the band of loadings in which the earlier essay found every seam helped.
Once the bend pulls the axial stress past twice the hoop stress, the wall begins to shorten round its circumference — the Poisson contraction of the axial pull outweighs the pressure’s hoop stretch — and a line appears along which the wall neither lengthens nor shortens. It appears at 90° to the axis, running round the tube, and as the bend grows it swings toward the axis, heading for the 54.7° of plain tension it would reach if the axial stress grew without end. With no pressure it starts at 54.7°. With pressure it has to come down from 90° to get there, and on the way it passes through 70°, 65°, 60° — the angles spiral mills use.
At a hoop stress of 50 N/mm², the 60° seam fails when the line on the stretched side is at 61.6°, almost exactly along it. At 100 N/mm² the seam fails earlier in the line’s descent, with the line at 77°. At 140 N/mm² the seam fails before any line has appeared. In each case the seam is failing where the parent’s help is close to nothing. The pressure has not protected the seam from the bend; it has made the bend begin its work from a hoop stress the seam must also carry.
Nearly on the line is enough
The earlier essay’s lead pictured the seam failing at the two points of each turn where it crosses the local unstretched line. The figure says where it actually fails.
The help the parent lends the band, at the moment the seam fails, is plotted round the tube. At every pressure it is close to one on the stretched side — 1.02 at 100 N/mm² — and rises away from it, to 1.32 a quarter of a turn round, where the bending stress is nothing and the wall carries only the pressure’s own field, whose help for a 60° seam is the 1.3 that gave the earlier essay its 78 per cent.
So the seam fails at its most stretched point, where the stress is largest, and the reason it fails there rather than somewhere the stress is a little lower is that the help there is almost none. The two effects point at the same place: the bend’s largest axial stress is also the stress that brings the unstretched line closest to the seam. The exact crossing of the seam and the line, where the help would be exactly one, need not happen before failure, and at 100 N/mm² it does not. Being near the line is enough to lose nearly all of the protection, because the help rises only slowly as the seam moves away from it.
The earlier question about borrowing a neighbour’s help has an answer too. The band condition is local: at each point along the seam, the parent either side fixes the band’s strain along its line, whatever the band is doing a quarter of a turn away. The band is not held by its neighbours along the seam but by the parent beside it, and the parent beside the most stretched point is in the most stretched loading. What a short length of yielding band might borrow from the unyielded band either side of it along the seam is a further restraint this model does not contain, and it would make the seam stronger, not weaker.
The envelope of pressure and bend
The parent barely notices the pressure: its bending strength falls from 310 N/mm² to 298 at a hoop stress of 100, because von Mises with a hoop tension beside an axial tension is forgiving. Both seams lose much more. The girth seam, running round the tube at 90° to its axis, falls from 214 to 164; the spiral seam at 60° from 186 to 167. At 100 N/mm² of hoop stress the spiral seam and the girth seam are within 2 per cent of each other, though under pressure alone the earlier essay found the girth seam lent twice its strength. In bending a girth seam is a band directly across the axial pull, the worst place for a soft zone in a stretched member, as two welds, and the one that decides found for a member pulled along its length.
The longitudinal seam is the exception, and it is complete. A seam along the axis is not crossed by any of the bend’s axial stress; it carries the pressure’s hoop stress across it and nothing else, so a bend can never fail it. That is the reverse of its situation under pressure, where the hoop stress falls squarely across it.
Where the girth seam and the spiral trade places
A pipeline made of spiral-welded tubes has both kinds of seam: the spiral along each tube, and a girth weld wherever two tubes are joined in the field. Under pressure alone the girth weld is the safer of the two by a wide margin. Under a bend the two curves in the last figure cross, at a hoop stress of about 84 N/mm², where both seams fail at a bending stress of 172.
Below that pressure the girth weld is the stronger in bending — 214 against 186 N/mm² with no pressure at all — and above it the spiral seam is, by a little. The difference either side of the crossing is never more than a few per cent, which is a practical result in itself: at a pipeline’s operating pressures the field girth weld and the mill’s spiral seam are about equally exposed to a bend, and an inspection that looks harder at one than the other is looking by habit rather than by the stresses.
The numbers that decide it are not the welds’ strengths, which are the same zone in the same alloy, but the angles. A girth seam sits at 90° to the axis, which the bend’s unstretched line passes through first when it appears; a 60° spiral seam is reached later in the line’s descent, after the axial stress has grown further. At the stretched fibre the spiral seam fails with an axial stress of 217 N/mm² at a hoop stress of 100, where with no pressure it failed at 186: the pressure delays the line’s arrival at 60° by making the bend do more work first, and then hands the seam a hoop stress of its own to carry. Which of those two effects wins depends on the pressure, and for a 60° seam they cancel near 84 N/mm².
Every seam angle under a bend
The seam’s share of the bending strength against its angle has a broad trough. Unpressurised, its bottom is at 54.7°, the uniaxial line, at 60 per cent. Under pressure the trough deepens and widens: at 100 N/mm² everything from about 40° to 90° keeps between 55 and 57 per cent, and the least is at 80°. The pressure has lowered every angle and moved the worst one toward the girth. There is no mill angle in the band from 50 to 70 degrees that a bend does not find; the earlier essay’s discovery that pressure protects all of them does not survive the bend for any of them.
Seams near the axis are the only safe ones. Below about 15° to the axis the bend’s axial stress crosses the seam so obliquely that the parent reaches its own strength first, and a seam at 10° would carry three quarters as much again as the parent before failing. Spiral mills do not wind at such angles.
Which side of the bend
The stretched side is where a steep seam fails, and it is not where every seam fails. A seam below about 55° to the axis, under pressure, fails on the side the bend squeezes. There the axial stress is compression and the hoop stress tension, and a seam at a shallow angle sees their difference as shear along itself. Shear is what the band condition weights most heavily — three times the shear’s square against three quarters of the normal stress’s — and the squeezed side has the largest difference between the two stresses anywhere round the tube.
Without pressure the squeezed side is just the stretched side’s mirror image and a shallow seam fails on the stretched side. The pressure makes the two sides different, and for shallow seams the difference favours the compressed side as the weak one: the worst stress is not where the worst bending is, and here it depends on the angle of a line welded into the wall.
What the tube’s wall is assumed to do
The tube is checked fibre by fibre at an elastic distribution of stress, as the earlier essays checked their loadings: each point’s stresses are the elastic ones, and a point reaching its strength ends the tube. A thin-walled aluminium tube in bending does not redistribute much before its most stretched fibre fails, but a tube of a ductile parent would yield first, and a bend that yielded the parent would change the stresses the seam sees. The band condition itself assumes the parent either side stays elastic, which holds here because the seam fails well below the parent’s strength.
The bending stress is taken as a pure function of position round the tube, with no ovalisation of the cross-section; a thin tube bent hard flattens, and its hoop stress then varies round the circumference as well. The pressure is held while the bend is applied, and the ends are closed. A pipe with open ends — held at its supports and carrying no axial pressure stress — starts its bend from a lower axial stress, so its unstretched line would appear later on the stretched side, needing more bend to pull the axial stress past twice the hoop stress; that is a different loading, along the same calculation.
A protection that belonged to one loading
The earlier essay’s protection was real and specific. A closed tube’s pressure produces one particular plane stress, twice as hard round as along, and that stress leaves no line in the wall unstretched at the angles mills wind. Any loading that changes the ratio of the two stresses can bring such a line back, and a bend is the commonest such loading a pipe meets. On its stretched side it pulls the wall along until the wall begins to shorten round its circumference, and the unstretched line that appears sweeps down through every angle mills use toward the 54.7° of plain tension. The seam is found by it at its most stretched point, with almost none of the protection left, and the pressure that gave the protection now only adds a hoop stress for the seam to carry.
Still open: the tube that is bent and then pressurised
Everything here held the pressure and then bent. A pipeline is often laid and bent first, cold-bent to its route or settled into a trench, and pressurised afterwards. A path of loading that bends the tube first and then raises the pressure crosses the plane of axial and hoop stress along a different route, and if the parent or the band yields on the way the order matters, because a yielded band remembers its strain. The soft zone that takes all the stretch found that a soft band in series concentrates the member’s deformation; whether a seam that has yielded a little in bending is then protected by the pressure that follows, as an elastic seam would be, or whether the strain it took in the bend leaves it without the reserve the pressure would have lent, is the question the order of a pipeline’s loads puts to the seam.
Named alongside this one
Essays reaching for the same objects. Nobody chose these; they are what the concept index makes visible.
- Both at once, and neither matters until it does bending stress · principal stress · yield criterion
- Each one stops the other failing hoop tension · yield criterion
- The angle that forgets the liner hoop tension · yield criterion
- The length a structure was never given hoop tension · restraint
- The pressure that switches at the hopper hoop tension · principal stress
- Two moments and a neutral axis that obeys neither bending stress · restraint
The objects this essay names
Each one links to every other essay that touches it.
Bending stressHeat-affected zoneHoop tensionPrincipal stressRestraintYield criterion